Logotype


search by parameters
analog search

catalogs
GOST Rus
Hikari
Hoya
O'Hara
Schott 2000
Special
Sumita

help

© 2003-2013 ACO department

Политика по обработке Персональных данных

 

E-LAK011 - Hikari

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.741000
ne = 1.744354
Vd = 52.67
Ve = 52.44
nF - nC = 0.014068
nF' - nC' = 0.014193
Coloring:
0.347 - 0.289 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.4046561 - 0.76819 mkm.
C1 = 2.97199342 C2 = -0.0152435249 C3 = 0.0202061158 C4 = 0.000875252167 C5 = -0.0000767180744 C6 = 0.00000484807195

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t-----
n s-----
n r1.734311
n C1.736733
n C'1.737411
n 0.63281.738045
n D1.740874
n d1.741000
n e1.744354
n F1.750801
n F'1.751605
n g1.758482
n h1.764882
n i-----
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t-----
PC,A'0.3447
Pd,C0.3032
Pe,C0.5417
Pg,d1.2427
Pg,F0.5459
Ph,g0.4548
Pi,g-----
PC',t-----
Pe,C'0.4935
PF',e0.5154
Pi,F'-----
 transmittance: 10 mm
τ0.290.01
τ0.30.09
τ0.310.26
τ0.320.49
τ0.330.65
τ0.340.77
τ0.350.86
τ0.360.912
τ0.370.948
τ0.380.971
τ0.390.982
τ0.40.99
τ0.420.997
τ0.440.999
τ0.460.999
τ0.480.999
τ0.50.999
τ0.550.999
τ0.60.999
τ0.650.999
τ0.70.999
τ0.80.999
τ0.90.999
τ10.999
τ1.20.999
τ1.40.999
τ1.60.999
τ1.80.987
τ20.962
τ2.20.88
τ2.40.62

  mechanical
Knoop hardness: 635
Abrasion: 50

  Chemical
Resistance to acids: 4

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30067