E-LAK12 - Hikari

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.677900
ne = 1.680816
Vd = 55.39
Ve = 55.15
nF - nC = 0.012237
nF' - nC' = 0.012343
Coloring:
0.337 - 0.278 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.4046561 - 0.76819 mkm.
C1 = 2.78094755 C2 = -0.0236624998 C3 = 0.00867653717 C4 = 0.00294181002 C5 = -0.000351554137 C6 = 0.0000184406503

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t-----
n s-----
n r1.672063
n C1.674185
n C'1.674776
n 0.63281.675329
n D1.677791
n d1.677900
n e1.680816
n F1.686422
n F'1.687120
n g1.693084
n h1.698633
n i-----
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t-----
PC,A'0.3499
Pd,C0.3035
Pe,C0.5419
Pg,d1.2408
Pg,F0.5443
Ph,g0.4534
Pi,g-----
PC',t-----
Pe,C'0.4935
PF',e0.5151
Pi,F'-----
 transmittance: 10 mm
τ0.290.01
τ0.30.09
τ0.310.3
τ0.320.52
τ0.330.69
τ0.340.81
τ0.350.88
τ0.360.929
τ0.370.957
τ0.380.971
τ0.390.98
τ0.40.984
τ0.420.988
τ0.440.989
τ0.460.992
τ0.480.994
τ0.50.995
τ0.550.997
τ0.60.998
τ0.650.998
τ0.70.999
τ0.80.999
τ0.90.999
τ10.999
τ1.20.999
τ1.40.992
τ1.60.995
τ1.80.982
τ20.96
τ2.20.88
τ2.40.7

  mechanical
Knoop hardness: 530
Abrasion: 155

  Chemical
Resistance to acids: 5

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30081