E-SSK8 - Hikari

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.617720
ne = 1.620671
Vd = 49.77
Ve = 49.48
nF - nC = 0.012409
nF' - nC' = 0.012542
Coloring:
0.375 - 0.341 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.4046561 - 0.76819 mkm.
C1 = 2.57047824 C2 = -0.0119686463 C3 = 0.0149712411 C4 = 0.00112845548 C5 = -0.000110413826 C6 = 0.00000739815032

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t-----
n s-----
n r1.611910
n C1.614001
n C'1.614589
n 0.63281.615140
n D1.617610
n d1.617720
n e1.620671
n F1.626410
n F'1.627132
n g1.633361
n h1.639260
n i-----
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t-----
PC,A'0.3362
Pd,C0.2996
Pe,C0.5375
Pg,d1.2604
Pg,F0.5601
Ph,g0.4754
Pi,g-----
PC',t-----
Pe,C'0.4901
PF',e0.5206
Pi,F'-----
 transmittance: 10 mm
τ0.340.03
τ0.350.25
τ0.360.57
τ0.370.77
τ0.380.88
τ0.390.932
τ0.40.961
τ0.420.982
τ0.440.987
τ0.460.99
τ0.480.994
τ0.50.996
τ0.550.998
τ0.60.996
τ0.650.993
τ0.70.996
τ0.80.999
τ0.90.999
τ10.999
τ1.20.999
τ1.40.999
τ1.60.996
τ1.80.984
τ20.971
τ2.20.93
τ2.40.87

  mechanical
Knoop hardness: 483
Abrasion: 184

  Chemical
Resistance to acids: 4

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30094