E-SSK2 - Hikari

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.622300
ne = 1.625092
Vd = 53.05
Ve = 52.76
nF - nC = 0.011728
nF' - nC' = 0.011847
Coloring:
0.353 - 0.332 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.4046561 - 0.76819 mkm.
C1 = 2.59124283 C2 = -0.014272062 C3 = 0.0123965569 C4 = 0.00153774031 C5 = -0.000159274472 C6 = 0.00000855211131

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t-----
n s-----
n r1.616781
n C1.618772
n C'1.619331
n 0.63281.619854
n D1.622196
n d1.622300
n e1.625092
n F1.630500
n F'1.631178
n g1.636991
n h1.642431
n i-----
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t-----
PC,A'0.3397
Pd,C0.3007
Pe,C0.5389
Pg,d1.2526
Pg,F0.5534
Ph,g0.4637
Pi,g-----
PC',t-----
Pe,C'0.4912
PF',e0.5188
Pi,F'-----
 transmittance: 10 mm
τ0.330.05
τ0.340.34
τ0.350.65
τ0.360.82
τ0.370.91
τ0.380.949
τ0.390.97
τ0.40.98
τ0.420.988
τ0.440.99
τ0.460.992
τ0.480.993
τ0.50.995
τ0.550.995
τ0.60.994
τ0.650.995
τ0.70.995
τ0.80.999
τ0.90.999
τ10.999
τ1.20.999
τ1.40.999
τ1.60.997
τ1.80.986
τ20.976
τ2.20.933
τ2.40.83

  mechanical
Knoop hardness: 437
Abrasion: 195

  Chemical
Resistance to acids: 4

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30089