E-SK11 - Hikari

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.563839
ne = 1.566055
Vd = 60.67
Ve = 60.43
nF - nC = 0.009292
nF' - nC' = 0.009366
Coloring:
0.336 - 0.300 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.4046561 - 0.76819 mkm.
C1 = 2.41034365 C2 = -0.0101286559 C3 = 0.0126748412 C4 = 0.000257347078 C5 = -0.00000624279133 C6 = 0.000000335932224

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t-----
n s-----
n r1.559380
n C1.561002
n C'1.561455
n 0.63281.561877
n D1.563756
n d1.563839
n e1.566055
n F1.570294
n F'1.570821
n g1.575317
n h1.579472
n i-----
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t-----
PC,A'0.3510
Pd,C0.3052
Pe,C0.5437
Pg,d1.2353
Pg,F0.5405
Ph,g0.4471
Pi,g-----
PC',t-----
Pe,C'0.4950
PF',e0.5129
Pi,F'-----
 transmittance: 10 mm
τ0.280.02
τ0.290.13
τ0.30.34
τ0.310.58
τ0.320.76
τ0.330.87
τ0.340.934
τ0.350.968
τ0.360.985
τ0.370.991
τ0.380.993
τ0.390.998
τ0.40.998
τ0.420.998
τ0.440.996
τ0.460.997
τ0.480.999
τ0.50.999
τ0.550.999
τ0.60.999
τ0.650.998
τ0.70.999

  mechanical
Knoop hardness: 492
Abrasion: 106

  Chemical
Resistance to acids: 3

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30076