E-SK5 - Hikari

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.589130
ne = 1.591427
Vd = 61.16
Ve = 60.91
nF - nC = 0.009632
nF' - nC' = 0.009708
Coloring:
0.334 - 0.294 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.4046561 - 0.76819 mkm.
C1 = 2.48616859 C2 = -0.00962090414 C3 = 0.0146866348 C4 = -0.000117877135 C5 = 0.0000443876615 C6 = -0.00000205228288

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t-----
n s-----
n r1.584499
n C1.586185
n C'1.586655
n 0.63281.587094
n D1.589044
n d1.589130
n e1.591427
n F1.595818
n F'1.596364
n g1.601028
n h1.605348
n i-----
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t-----
PC,A'0.3520
Pd,C0.3056
Pe,C0.5441
Pg,d1.2352
Pg,F0.5409
Ph,g0.4484
Pi,g-----
PC',t-----
Pe,C'0.4953
PF',e0.5125
Pi,F'-----
 transmittance: 10 mm
τ0.290.02
τ0.30.14
τ0.310.36
τ0.320.58
τ0.330.75
τ0.340.86
τ0.350.918
τ0.360.957
τ0.370.972
τ0.380.985
τ0.390.988
τ0.40.992
τ0.420.993
τ0.440.994
τ0.460.995
τ0.480.996
τ0.50.997
τ0.550.999
τ0.60.999
τ0.650.998
τ0.70.999

  mechanical
Poisson coef.: 0.252
Rigidity: 34.6 Pa*108
Young module: 86.7 Pa*108
Knoop hardness: 611
Abrasion: 126

  Chemical
Resistance to acids: 4

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30069