E-SK4 - Hikari

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.612716
ne = 1.615203
Vd = 58.73
Ve = 58.45
nF - nC = 0.010432
nF' - nC' = 0.010524
Coloring:
0.345 - 0.310 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.4046561 - 0.76819 mkm.
C1 = 2.55935739 C2 = -0.0101666557 C3 = 0.01458787 C4 = 0.00036544107 C5 = -0.0000159151229 C6 = 0.00000099861439

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t-----
n s-----
n r1.607750
n C1.609549
n C'1.610052
n 0.63281.610523
n D1.612623
n d1.612716
n e1.615203
n F1.619981
n F'1.620577
n g1.625668
n h1.630390
n i-----
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t-----
PC,A'0.3455
Pd,C0.3035
Pe,C0.5419
Pg,d1.2415
Pg,F0.5451
Ph,g0.4526
Pi,g-----
PC',t-----
Pe,C'0.4936
PF',e0.5151
Pi,F'-----
 transmittance: 10 mm
τ0.290.01
τ0.30.07
τ0.310.2
τ0.320.35
τ0.330.53
τ0.340.72
τ0.350.86
τ0.360.94
τ0.370.983
τ0.380.999
τ0.390.999
τ0.40.999
τ0.420.999
τ0.440.999
τ0.460.999
τ0.480.999
τ0.50.999
τ0.550.999
τ0.60.999
τ0.650.999
τ0.70.999
τ0.80.999
τ0.90.999
τ10.999
τ1.20.999
τ1.40.999
τ1.60.999
τ1.80.999
τ20.989
τ2.20.944
τ2.40.848

  mechanical
Knoop hardness: 598
Abrasion: 144

  Chemical
Resistance to acids: 4

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30072