E-BASF7 - Hikari

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.701540
ne = 1.705586
Vd = 41.16
Ve = 40.88
nF - nC = 0.017041
nF' - nC' = 0.017256
Coloring:
0.388 - 0.356 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.4046561 - 0.76819 mkm.
C1 = 2.83515039 C2 = -0.0178508143 C3 = 0.0153978598 C4 = 0.00371905515 C5 = -0.000488482182 C6 = 0.0000329017911

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t-----
n s-----
n r1.693698
n C1.696497
n C'1.697290
n 0.63281.698034
n D1.701390
n d1.701540
n e1.705586
n F1.713539
n F'1.714546
n g1.723338
n h1.731898
n i-----
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t-----
PC,A'0.3260
Pd,C0.2958
Pe,C0.5333
Pg,d1.2791
Pg,F0.5750
Ph,g0.5023
Pi,g-----
PC',t-----
Pe,C'0.4868
PF',e0.5257
Pi,F'-----
 transmittance: 10 mm
τ0.350.03
τ0.360.23
τ0.370.51
τ0.380.71
τ0.390.83
τ0.40.902
τ0.420.964
τ0.440.984
τ0.460.993
τ0.480.999
τ0.50.999
τ0.550.999
τ0.60.999
τ0.650.999
τ0.70.999
τ0.80.999
τ0.90.999
τ10.999
τ1.20.999
τ1.40.997
τ1.60.999
τ1.80.992
τ20.988
τ2.20.962
τ2.40.88

  mechanical
Knoop hardness: 517
Abrasion: 148

  Chemical
Resistance to acids: 3

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30083