 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.669981
ne = 1.674033
Vd = 39.20
Ve = 38.92
nF - nC = 0.017087
nF' - nC' = 0.017314
Coloring:
0.35 - 0.40 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.4046561 - 1.01398 mkm.
C1 = 2.7157255 C2 = -0.0085850692 C3 = 0.02429997 C4 = 0.00065374795 C5 = -0.0000026114074 C6 = 0.0000037821413

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t1.652619
n s1.656564
n r1.662162
n C1.664947
n C'1.665737
n 0.63281.666479
n D1.669831
n d1.669981
n e1.674033
n F1.682034
n F'1.683052
n g1.691941
n h1.700519
n i-----
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t0.7214
PC,A'0.3224
Pd,C0.2945
Pe,C0.5317
Pg,d1.2851
Pg,F0.5797
Ph,g0.5020
Pi,g-----
PC',t0.7676
Pe,C'0.4854
PF',e0.5278
Pi,F'-----
 transmittance: 10 mm
τ0.350.027
τ0.360.255
τ0.370.576
τ0.380.775
τ0.390.873
τ0.40.922
τ0.420.96
τ0.440.974
τ0.460.981
τ0.480.982
τ0.50.985
τ0.550.99
τ0.60.992
τ0.650.994
τ0.70.995
τ0.80.998
τ1.060.998
τ1.50.998
τ20.982
 transmittance: 25 mm
τ0.360.033
τ0.370.252
τ0.380.529
τ0.390.714
τ0.40.817
τ0.420.903
τ0.440.937
τ0.460.954
τ0.480.957
τ0.50.964
τ0.550.975
τ0.60.982
τ0.650.985
τ0.70.989
τ0.80.996
τ1.060.996
τ1.50.996
τ20.957

  mechanical
Poisson coef.: 0.261
Rigidity: 295 Pa*108
Young module: 745 Pa*108
Knoop hardness: 574
Abrasion: 190

  Chemical
Climatic resistance: 1
Resistance to acids: 3

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30087