KF3 - Sumita

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.514537
ne = 1.516781
Vd = 54.63
Ve = 54.35
nF - nC = 0.009418
nF' - nC' = 0.009507
Coloring:
0.30 - 0.32 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.3650146 - 1.01398 mkm.
C1 = 2.2595072 C2 = -0.0087017925 C3 = 0.011691949 C4 = 0.00050751817 C5 = -0.000040895778 C6 = 0.0000026801217

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t1.504120
n s1.506704
n r1.510078
n C1.511690
n C'1.512142
n 0.63281.512565
n D1.514453
n d1.514537
n e1.516781
n F1.521109
n F'1.521650
n g1.526290
n h1.530629
n i1.538150
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t0.8037
PC,A'0.3425
Pd,C0.3022
Pe,C0.5405
Pg,d1.2479
Pg,F0.5501
Ph,g0.4606
Pi,g1.2591
PC',t0.8517
Pe,C'0.4925
PF',e0.5169
Pi,F'1.7518
 transmittance: 10 mm
τ0.30.122
τ0.310.6
τ0.320.839
τ0.330.936
τ0.340.967
τ0.350.977
τ0.360.982
τ0.370.982
τ0.380.985
τ0.390.988
τ0.40.988
τ0.420.988
τ0.440.988
τ0.460.988
τ0.480.99
τ0.50.99
τ0.550.991
τ0.60.994
τ0.650.994
τ0.70.995
τ0.80.998
τ1.060.994
τ1.50.985
τ20.929
 transmittance: 25 mm
τ0.310.279
τ0.320.646
τ0.330.848
τ0.340.92
τ0.350.944
τ0.360.957
τ0.370.957
τ0.380.964
τ0.390.971
τ0.40.971
τ0.420.971
τ0.440.971
τ0.460.971
τ0.480.975
τ0.50.975
τ0.550.978
τ0.60.985
τ0.650.985
τ0.70.989
τ0.80.996
τ1.060.985
τ1.50.964
τ20.832

  mechanical
Poisson coef.: 0.218
Rigidity: 261 Pa*108
Young module: 637 Pa*108
Knoop hardness: 497
Abrasion: 120

  Chemical
Climatic resistance: 1
Resistance to acids: 2

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 300107