K-SK16RH - Sumita

 Diagram n (λ)    n calculation    Diagram τ (λ)    τ calculation    Analogue search

  Main parameters
nd = 1.620407
ne = 1.622862
Vd = 60.28
Ve = 60.04
nF - nC = 0.010292
nF' - nC' = 0.010373
Coloring:
0.29 - 0.35 mkm.

  Coefficients of dispertion formulas
Type: Schott
Spectral range: 0.3650146 - 1.01398 mkm.
C1 = 2.584811 C2 = -0.011486919 C3 = 0.014859018 C4 = 0.00021677739 C5 = -0.00000024466918 C6 = 0.00000031088303

  Refraction index
n 2.3254-----
n 1.9701-----
n 1.5296-----
n 1.06-----
n t1.608619
n s1.611628
n r1.615462
n C1.617262
n C'1.617764
n 0.63281.618233
n D1.620315
n d1.620407
n e1.622862
n F1.627554
n F'1.628138
n g1.633115
n h1.637722
n i1.645569
n 0.3341-----
n 0.3126-----
n 0.2967-----
n 0.2804-----
n 0.2483-----
  Relative partial dispertion
PC,t0.8397
PC,A'0.3519
Pd,C0.3055
Pe,C0.5441
Pg,d1.2346
Pg,F0.5402
Ph,g0.4476
Pi,g1.2101
PC',t0.8885
Pe,C'0.4953
PF',e0.5125
Pi,F'1.6937
 transmittance: 10 mm
τ0.280.01
τ0.290.086
τ0.30.251
τ0.310.447
τ0.320.625
τ0.330.772
τ0.340.86
τ0.350.915
τ0.360.957
τ0.370.978
τ0.380.985
τ0.390.997
τ0.40.997
τ0.420.997
τ0.440.997
τ0.460.998
τ0.480.998
τ0.50.998
τ0.550.998
τ0.60.998
τ0.650.998
τ0.70.998
τ0.80.998
τ1.060.992
τ1.50.978
τ20.953
 transmittance: 25 mm
τ0.30.031
τ0.310.134
τ0.320.309
τ0.330.525
τ0.340.686
τ0.350.801
τ0.360.896
τ0.370.947
τ0.380.964
τ0.390.992
τ0.40.992
τ0.420.992
τ0.440.992
τ0.460.996
τ0.480.996
τ0.50.996
τ0.550.996
τ0.60.996
τ0.650.996
τ0.70.996
τ0.80.996
τ1.060.982
τ1.50.947
τ20.887

  mechanical
Poisson coef.: 0.266
Rigidity: 351 Pa*108
Young module: 888 Pa*108
Knoop hardness: 624
Abrasion: 130

  Chemical
Climatic resistance: 1
Resistance to acids: 5

 Temperature coefficient of linear expansion
Temp. range, CValue, 1/C*10^-7
100 ~ 30072